Abstract
In this work, the self-assembled morphologies obtained for poly(styrene-b-butadiene-b-styrene) (SBS) and poly(styrene-b-isoprene-b-styrene) (SIS) ABA-type copolymers were investigated before and after hydrogenation of the polydiene block, which led to poly(styrene-b-ethylene)/poly(ethylene-b-styrene) (SEES) and poly(styrene-b-ethylene)/poly(propylene-b-styrene) (SEPS) copolymers, respectively. The evaluation of different morphologies was carried out using atomic force microscopy (AFM), analyzing the effect of various parameters such as the solvent and polymer concentrations employed for film casting (toluene, cyclohexane, or tetrahydrofurane with concentrations of 1 and 3 wt%), together with that of the annealing treatment (thermal annealing at room temperature, and 60, 80, and 100 degrees C). The effect of these parameters in combination with the chemical nature of the polydiene block led to different morphologies with different topographic aspects affecting the roughness (Ra) of the film.